4 Therma-Tech
Incomplete Fill
Melt and/or mold
too cold
• Increase nozzle and barrel temperatures
• Increase pack and hold pressure
• Increase nozzle tip diameter
• Check thermocouples and heater bands
Mold design
• Enlarge or widen vents and increase number of vents
• Check that vents are unplugged
• Check that gates are unplugged
• Enlarge gates and/or runners
• Perform short shots to determine fill pattern and
verify proper vent location
• Increase wall thickness to move gas trap to
parting line
Shot size
• Increase cushion
• Decrease transfer position
Brittleness
Low melt
temperature
• Measure melt temperature with pyrometer
Degraded/
overheated
material
• Decrease melt temperature
• Decrease back pressure
• Use smaller barrel/excessive residence time
• Decrease screw rpm
Gate location
and/or size
• Relocate gate to nonstress area
• Increase gate size to allow higher flow rate and lower
molded in stress
Fibers on Surface
(Splay)
Melt temperature
too low
• Increase injection speed
• Increase screw rpm
Insufficient packing
• Increase pack and hold pressure, and time
Processing Guide 5
Sink Marks
Part geometry
too thick
• Reduce wall thickness
• Reduce rib thickness
• Maintain nominal wall thickness
Melt too hot • Decrease nozzle and barrel temperatures
Insufficient
material volume
• Increase pack pressure/time
Flash
Injection pressure
too high
• Decrease injection pressure
• Increase clamp pressure
• Increase transfer position
Excess
material volume
• Decrease pack pressure
• Decrease shot size
Melt and/or mold
too hot
• Decrease screw speed
Excessive Shrink Too much
orientation
• Increase packing time and pressure
• Increase hold pressure
• Decrease melt temperature
• Decrease injection speed
• Decrease screw rpm
• Increase venting
Not Enough Shrink Too little
orientation
• Decrease packing pressure and time
• Decrease hold pressure
• Increase injection speed
• Increase screw rpm
• Decrease cooling time
6 Therma-Tech
Burning
Melt and/or mold
too cold
Mold design • Clean, widen and increase number of vents
• Increase gate size or number of gates
Moisture • Verify material is dried at proper conditions
Nozzle Drool Nozzle temperature
too hot
• Decrease nozzle temperature
• Decrease back pressure
• Increase screw decompression
• Verify material has been dried at proper conditions
Weld Lines
Melt front temperatures
are too low
• Increase pack and hold pressure
• Increase vent width and locations
Mold design
• Perform short shots to determine fill pattern
and verify proper vent location
• Add vents and/or false ejector pin
• Move gate location
Warp
Excessive orientation
• Decrease injection pressure and injection rate
Mold design • Increase number of gates
Sticking in Mold
Cavities are
overpacked
• Decrease injection rate and pressure
• Decrease pack and hold pressure
Mold design • Increase draft angle
Part is too hot
1.844.4AVIENT
www.avient.com
Copyright © 2020, Avient Corporation.
https://www.avient.com/sites/default/files/2023-04/Fiber Colorants and Additives Brochure.pdf
The reliable low liquid level
detection system alerts operators when product
is running low; adding additional product does
not require stopping the machine, so continuous
production is possible without any loss of part color.
1.844.4AVIENT
www.avient.com
Copyright © 2023, Avient Corporation.
https://www.avient.com/sites/default/files/2022-06/MEVOPUR Bio-based Solutions Application Bulletin_CN %281%29.pdf
1.844.4AVIENT
www.avient.com
版权所有© 2022埃万特公司。
https://www.avient.com/sites/default/files/2022-08/MEVOPUR Special Effect Colors Application Bulletin_CN.pdf
可根据要求提供FDA/EU合规信息
1.844.4AVIENT
www.avient.com
版权所有© 2022埃万特公司。
https://www.avient.com/sites/default/files/2022-01/ColorMatrix_ Optica_ PET.pdf
回收应用 APR认证 2021 2021
1.844.4AVIENT
www.avient.com
版权所有©2021 埃万特公司。
https://www.avient.com/sites/default/files/2020-08/colormatrix-lactra-sx.pdf
www.avient.com
版权所有© 2020埃万特公司。
https://www.avient.com/sites/default/files/2021-09/mevopur-colors-for-ophthalmic-closures-application-bulletin-cn.pdf
1.844.4AVIENT
www.avient.com
版权所有© 2021埃万特公司。
https://www.avient.com/sites/default/files/2020-08/cai-wire-and-cable-product-selection-brochure-cn.pdf
海蓝色
适用于汽车电线的 ONCOLORTM 解决方案
适用于交联材料如 XLPE 的 EVA 色母料,以及适用于 T1、T2 和 T3 耐热等级要求的 PVC 色母料
建议使用量为 1-2%,使用量可能因具体用途、工艺、设备和树脂级别不同而存在差异
海蓝色
蓝色 (浅蓝)
适用于通信电缆和光缆应用的 PVC 和 PBT 色母料
适用于发泡和固体绝缘应用的 PE 色母料
为交联材料如 XLPE 专门设计的 EVA 色母料
所有材料建议使用量为 1-2%,使用量可能因具体用途、工艺、设备和合成树脂级不同而存在差异
适用于通信线缆应用的 ONCOLORTM 解决方案
海蓝色
蓝色 (浅蓝)
海蓝色
海蓝色
适用于室外线缆应用的抗紫外色母料
建议 PE 材料使用量为 2%,PVC 材料使用量为 3%,使用量可能因具体用途、工艺、设
备和树脂级别不同而存在差异
www.avient.com
版权所有© 2020埃万特公司。
https://www.avient.com/sites/default/files/2025-04/ColorMatrix_ Amosorb_ 4020L_CN.pdf
主要优势
• 优异的可回收性
• 与rPET相容(适合用于>25% rPET含量)
• 非尼龙基
• 即时起效的吸氧反应
• 通过灵活调节添加比(LDR)实现长期保质期
• 即使在较高LDR下,瓶身外观依然出色
• 可轻松与现有单层注塑设备一起使用
• 适用于多层注塑设备
产品公告
1.844.4AVIENT
www.avient.com
版权所有©2025埃万特公司。